Timber · Glued laminated timber, homogeneous · orthotropic

GL24h

EN 14080:2013 · strength class

GL24h is a homogeneous glued laminated timber class to EN 14080:2013. Its characteristic bending strength is 24 MPa. Along the fibres E₁ = 11.5 GPa; across them E₂ = 0.3 GPa.

Record
glulam-gl24h
Library
v1.1.0
Properties
19
Sources
1
Build check
passed ✓
Viewing as
guest
+ Compare Cite Download · PRO
E₁ · Modulus, direction 1 11.5GPa mean[1]
f_m,k · Bending strength 24MPa char[1]
f_t,0,k · Tension parallel to grain 19.2MPa char[1]
ρ · Density 420kg/m³ mean[1]

Elastic constants

orthotropic
SymbolPropertyValueUnitBasisRef.
E₁ Modulus, direction 1 ⓘ E_0,g,mean 11.5 GPa mean [1]
E₀,₀₅ Modulus parallel to grain, 5 % fractile 9.6 GPa char [1]
E₂ Modulus, direction 2 ⓘ E_90,g,mean 0.3 GPa mean [1]
E₃ Modulus, direction 3 ⓘ E_90,g,mean 0.3 GPa mean [1]
G₁₂ Shear modulus 1-2 ⓘ G_g,mean 0.65 GPa mean [1]
G₁₃ Shear modulus 1-3 ⓘ G_g,mean 0.65 GPa mean [1]
G₀₅ Shear modulus, 5 % fractile 0.54 GPa char [1]
E₉₀,₀₅ Modulus perpendicular to grain, 5 % fractile 0.25 GPa char [1]
G₂₃ Shear modulus 2-3 ⓘ G_r,g,mean, rolling shear 0.065 GPa mean [1]
G_r Rolling shear modulus 0.065 GPa mean [1]

Physical, thermal and electrical

at 20 °C
SymbolPropertyValueUnitBasisRef.
ρ Density 420 kg/m³ mean [1]
ρ_k Density, characteristic (5 % fractile) 385 kg/m³ char [1]

Strength

a band applies up to and including its upper limit
SymbolPropertyValueUnitBasisRef.
f_m,k Bending strength 24 MPa char [1]
f_t,0,k Tension parallel to grain 19.2 MPa char [1]
f_t,90,k Tension perpendicular to grain 0.5 MPa char [1]
f_c,90,k Compression perpendicular to grain 2.5 MPa char [1]
f_v,k Shear strength 3.5 MPa char [1]
f_c,0,k Compression parallel to grain 24 MPa char [1]
f_r,k Rolling shear strength 1.2 MPa char [1]

Notes

  • EN 338 and EN 14080 give no Poisson's ratios; a 3D analysis needs them from another source.

Sources

every value names one
  1. EN 14080:2013, Timber structures — Glued laminated timber, Tables 4 and 5Copies checked: 1, 2, 3, 4

min product standard minimum char characteristic design code value for design typical datasheet or textbook derived worked out here, formula shown

Cite this page

for reports and papers

BadgerMecX Materials (2026). GL24h — material properties, EN 14080:2013. Library v1.1.0, record glulam-gl24h. https://badgermecx.com/materials/glulam-gl24h/ (accessed 2026-11-26).

@misc{badgermecx_glulamgl24h,
  title  = {GL24h -- material properties, EN 14080:2013},
  author = {{BadgerMecX Materials}},
  year   = {2026},
  note   = {Library v1.1.0, record glulam-gl24h},
  url    = {https://badgermecx.com/materials/glulam-gl24h/}
}

Export and related