GL20c vs GL30c

GL30c is 1.2 times as stiff as GL20c. It is 1.1 times as dense. Per unit mass GL30c is 1.1 times as stiff. Strength: f_m,k = 20 MPa for GL20c, f_m,k = 30 MPa for GL30c.

Side by side

ratio = GL30c / GL20c · log scale
Property GL20c GL30cUnitRatio¼×1×4×
E₁ Modulus, direction 1 10.4 13 GPa 1.25×
E₂ Modulus, direction 2 0.3 0.3 GPa 1×
E₃ Modulus, direction 3 0.3 0.3 GPa 1×
G₁₂ Shear modulus 1-2 0.65 0.65 GPa 1×
G₁₃ Shear modulus 1-3 0.65 0.65 GPa 1×
E₀,₀₅ Modulus parallel to grain, 5 % fractile 8.6 10.8 GPa 1.26×
G₀₅ Shear modulus, 5 % fractile 0.54 0.54 GPa 1×
ρ Density 390 430 kg/m³ 1.1×
ρ_k Density, characteristic (5 % fractile) 355 390 kg/m³ 1.1×
f_m,k Bending strength 20 30 MPa 1.5×
f_t,0,k Tension parallel to grain 15 19.5 MPa 1.3×
f_t,90,k Tension perpendicular to grain 0.5 0.5 MPa 1×
f_c,0,k Compression parallel to grain 18.5 24.5 MPa 1.32×
f_c,90,k Compression perpendicular to grain 2.5 2.5 MPa 1×
f_v,k Shear strength 3.5 3.5 MPa 1×
E/ρ Specific stiffness E/ρ · derived 26.67 30.23 MJ/kg 1.13×
c₀ Bar wave speed √(E/ρ) · derived 5164 5498 m/s 1.06×
f/ρ Specific strength f/ρ · derived 51.28 69.77 kJ/kg 1.36×

Values at the first thickness band or product form of each material (EN 14080:2013; EN 14080:2013). A minimum and a characteristic value are not the same kind of number — read the ratio as a guide. Each material's page lists every band and every source.