C20/25 vs C30/37

C30/37 is 1.1 times as stiff as C20/25. Their densities are about the same. Per unit mass C30/37 is 1.1 times as stiff. Strength: f_ck = 20 MPa for C20/25, f_ck = 30 MPa for C30/37.

Side by side

ratio = C30/37 / C20/25 · log scale
Property C20/25 C30/37UnitRatio¼×1×4×
E Young's modulus 30 33 GPa 1.1×
G Shear modulus 12.5 13.75 GPa 1.1×
ν Poisson's ratio 0.2 0.2 – 1×
ρ Density 2447 2447 kg/m³ 1×
γ Weight density 24 24 kN/m³ 1×
α Coefficient of thermal expansion 10 10 10⁻⁶/K 1×
f_ck Characteristic cylinder strength 20 30 MPa 1.5×
f_ck,cube Characteristic cube strength 25 37 MPa 1.48×
f_cm Mean cylinder strength 28 38 MPa 1.36×
f_ctm Mean tensile strength 2.2 2.9 MPa 1.32×
f_ctk,0.05 Tensile strength, 5 % fractile 1.5 2 MPa 1.33×
f_ctk,0.95 Tensile strength, 95 % fractile 2.9 3.8 MPa 1.31×
ε_c1 Strain at peak stress 2 2.2 ‰ 1.1×
ε_cu1 Ultimate strain 3.5 3.5 ‰ 1×
ε_c2 Strain at peak, parabola–rectangle 2 2 ‰ 1×
ε_cu2 Ultimate strain, parabola–rectangle 3.5 3.5 ‰ 1×
n Exponent, parabola–rectangle 2 2 – 1×
ε_c3 Strain at peak, bilinear 1.75 1.75 ‰ 1×
ε_cu3 Ultimate strain, bilinear 3.5 3.5 ‰ 1×
E/ρ Specific stiffness E/ρ · derived 12.26 13.48 MJ/kg 1.1×
c₀ Bar wave speed √(E/ρ) · derived 3501 3672 m/s 1.05×
f/ρ Specific strength f/ρ · derived 8.172 12.26 kJ/kg 1.5×

Values at the first thickness band or product form of each material (EN 1992-1-1; EN 1992-1-1). A minimum and a characteristic value are not the same kind of number — read the ratio as a guide. Each material's page lists every band and every source.