C16/20 vs C90/105

C90/105 is 1.5 times as stiff as C16/20. Their densities are about the same. Per unit mass C90/105 is 1.5 times as stiff. Strength: f_ck = 16 MPa for C16/20, f_ck = 90 MPa for C90/105.

Side by side

ratio = C90/105 / C16/20 · log scale
Property C16/20 C90/105UnitRatio¼×1×4×
E Young's modulus 29 44 GPa 1.52×
G Shear modulus 12.08 18.33 GPa 1.52×
ν Poisson's ratio 0.2 0.2 – 1×
ρ Density 2447 2447 kg/m³ 1×
γ Weight density 24 24 kN/m³ 1×
α Coefficient of thermal expansion 10 10 10⁻⁶/K 1×
f_ck Characteristic cylinder strength 16 90 MPa 5.62×
f_ck,cube Characteristic cube strength 20 105 MPa 5.25×
f_cm Mean cylinder strength 24 98 MPa 4.08×
f_ctm Mean tensile strength 1.9 5 MPa 2.63×
f_ctk,0.05 Tensile strength, 5 % fractile 1.3 3.5 MPa 2.69×
f_ctk,0.95 Tensile strength, 95 % fractile 2.5 6.6 MPa 2.64×
ε_c1 Strain at peak stress 1.9 2.8 ‰ 1.47×
ε_cu1 Ultimate strain 3.5 2.8 ‰ 0.8×
ε_c2 Strain at peak, parabola–rectangle 2 2.6 ‰ 1.3×
ε_cu2 Ultimate strain, parabola–rectangle 3.5 2.6 ‰ 0.743×
n Exponent, parabola–rectangle 2 1.4 – 0.7×
ε_c3 Strain at peak, bilinear 1.75 2.3 ‰ 1.31×
ε_cu3 Ultimate strain, bilinear 3.5 2.6 ‰ 0.743×
E/ρ Specific stiffness E/ρ · derived 11.85 17.98 MJ/kg 1.52×
c₀ Bar wave speed √(E/ρ) · derived 3442 4240 m/s 1.23×
f/ρ Specific strength f/ρ · derived 6.538 36.78 kJ/kg 5.62×

Values at the first thickness band or product form of each material (EN 1992-1-1; EN 1992-1-1). A minimum and a characteristic value are not the same kind of number — read the ratio as a guide. Each material's page lists every band and every source.