EN AW-6063 T66 and EN AW-6061 T4 are about equally stiff. Their densities are about the same. Per unit mass they are about equally stiff (25.93 and 25.93 MJ/kg). Strength: f_o = 110 MPa for EN AW-6061 T4, f_o = 200 MPa for EN AW-6063 T66.
ratio = EN AW-6063 T66 / EN AW-6061 T4 · log scale
Property
EN AW-6061 T4
EN AW-6063 T66
Unit
Ratio
¼×1×4×
E Young's modulus
70
70
GPa
1×
G Shear modulus
27
27
GPa
1×
ν Poisson's ratio
0.3
0.3
–
1×
ρ Density
2700
2700
kg/m³
1×
α Coefficient of thermal expansion
23
23
10⁻⁶/K
1×
λ Thermal conductivity
170
—
W/(m·K)
—
σ_e Electrical conductivity
22
—
MS/m
—
f_u Tensile strength (R_m)
180
245
MPa
1.36×
f_o 0.2 % proof strength
110
200
MPa
1.82×
f_o,haz 0.2 % proof strength in the heat-affected zone
95
75
MPa
0.789×
f_u,haz Tensile strength in the heat-affected zone
150
130
MPa
0.867×
E/ρ Specific stiffness E/ρ · derived
25.93
25.93
MJ/kg
1×
c₀ Bar wave speed √(E/ρ) · derived
5092
5092
m/s
1×
f/ρ Specific strength f/ρ · derived
40.74
74.07
kJ/kg
1.82×
Values at the first thickness band or product form of each material (EN 1999-1-1 · t ≤ 25 mm · EP, ET, ER/B; EN 1999-1-1 · t ≤ 10 mm · EP, ET, ER/B). A minimum and a characteristic value are not the same kind of number — read the ratio as a guide. Each material's page lists every band and every source.
COOKIES
We use a few cookies to see which pages engineers actually read and where they get stuck, and to tell whether our Google Search ads led to a sign-up or a purchase. No retargeting, nothing that follows you to other sites. They only start if you accept; reject and they stay off, and the site works exactly the same.